Carbon fibre reinforced filament with a PLA matrix.
- Polymer matrix
- PLA
- Filament diameter
- 1.75 ± 0.03 mm
- Net filament weight
- 1 kg
Price confirmed by quotation
We confirm pricing, supply and sample availability on request.

Application example
Check enclosure fit before assembly.
Use an enclosure prototype to check screw bosses, lid fit and component clearances on the first part. Refer to the data sheet when assessing heated areas and service temperature.
- Tensile strength · XY
- 50 ± 1 MPa
- Tensile strength · Z
- 17 ± 1 MPa
- HDT · ISO 75 (1.80 MPa)
- 55.3 °C
Material selection
Compare the technical data.
The supplier reported PETG-CF and PLA-CF results under the same test methods. The specimens were printed at different nozzle and bed temperatures.
| Property and method | PETG-CFAvailable from supplier | PLA-CFAvailable from supplier | PA6-CFIn testing | PPS-CFIn testing |
|---|---|---|---|---|
| Measured properties | ||||
| Tensile strength · XYISO 527 / GB/T 1040 | 66 ± 2 MPa | 50 ± 1 MPa | Data pending | Data pending |
| Tensile strength · ZISO 527 / GB/T 1040 | 19 ± 1 MPa | 17 ± 1 MPa | Data pending | Data pending |
| Flexural modulus · XYISO 178 / GB/T 9341 | 5,825 ± 101 MPa | 6,716 ± 163 MPa | Data pending | Data pending |
| HDTISO 75 · 1.80 MPa | 70.5 °C | 55.3 °C | Data pending | Data pending |
| DensityISO 1183 | 1.265 g/cm³ | 1.289 g/cm³ | Data pending | Data pending |
| Recommended print conditions | ||||
| Nozzle temperature | 230–260 °C | 200–230 °C | Data pending | Data pending |
| Bed temperature | 60–70 °C | 55–65 °C | Data pending | Data pending |
| Drying before printing | 65 °C for 6–12 hours | 55 °C for 6–12 hours | Data pending | Data pending |
HDT measures deflection under the specified load. Validate the part’s service temperature under its intended operating conditions.
Product format
- Filament diameter
- 1.75 ± 0.03 mm
- Net filament weight
- 1 kg
- Packaging
- Vacuum-sealed bag and carton
- Spool material
- Cardboard
- Empty spool weight
- 146 ± 1 g
- Spool dimensions
- Outer Ø 200 mm · inner Ø 88.5 mm · width 65.5 mm
- Carbon fibre content
- Unspecified in the TDS
- Country of origin
- China
Recommended printing settings
- Pre-print drying
- 55 °C for 6–12 hours
- Nozzle temperature
- 200–230 °C
- Bed temperatureTextured PEI plate
- 55–65 °C
- Chamber temperature
- < 45 °C
- Printer type
- Open-frame and enclosed
- Nozzle material
- Hardened steel or tungsten carbide
- Nozzle diameter
- 0.4 / 0.6 / 0.8 mm
- Print speed
- 30–300 mm/s
- Volumetric flow
- 3–32 mm³/s
- Cooling fan speed
- 50–100 %
- Optional annealing
- 55–60 °C for 6–12 hours
Physical and thermal properties
- DensityISO 1183
- 1.289 g/cm³
- Glass transition temperature (Tg)DSC, 10 °C/min
- 60.5 °C
- Melting temperatureDSC, 10 °C/min
- 159.4 °C
- Vicat softening temperatureISO 306 / GB/T 1633
- 63.2 °C
- Heat deflection temperature (HDT)ISO 75 · 1.80 MPa
- 55.3 °C
- Heat deflection temperature (HDT)ISO 75 · 0.45 MPa
- 57.4 °C
HDT is the deflection temperature measured at the specified test load. Assess suitability under the part’s actual service conditions.
Avoid exposing printed parts to temperatures above 55 °C.
Mechanical properties of printed specimens
- Tensile strength · XYISO 527 / GB/T 1040
- 50 ± 1 MPa
- Tensile strength · ZISO 527 / GB/T 1040
- 17 ± 1 MPa
- Young’s modulus · XYISO 527 / GB/T 1040
- 5,774 ± 289 MPa
- Young’s modulus · ZISO 527 / GB/T 1040
- 2,363 ± 267 MPa
- Elongation at break · XYISO 527 / GB/T 1040
- 1.3 ± 0.1 %
- Elongation at break · ZISO 527 / GB/T 1040
- 0.9 ± 0.1 %
- Flexural strength · XYISO 178 / GB/T 9341
- 79 ± 2 MPa
- Flexural strength · ZISO 178 / GB/T 9341
- 28 ± 1 MPa
- Flexural modulus · XYISO 178 / GB/T 9341
- 6,716 ± 163 MPa
- Flexural modulus · ZISO 178 / GB/T 9341
- 2,260 ± 22 MPa
- Unnotched impact strength · XYISO 179 / GB/T 1043
- 12.5 ± 0.7 kJ/m²
- Notched impact strength · XYISO 179 / GB/T 1043
- 3.1 ± 0.1 kJ/m²
- Impact strength · ZISO 179 / GB/T 1043
- 4.9 ± 0.4 kJ/m²
Reference results from the manufacturer’s data sheet. Values may vary with printer, drying and print settings.
Test specimen preparation
- Printer
- Bambu Lab H2D
- Nozzle temperature
- 230 °C
- Nozzle diameter
- 0.4 mm
- Bed temperature
- 55 °C
- Layer height
- 0.2 mm
- Print speed
- XY 150 mm/s · Z 60 mm/s
- Infill
- 100% · concentric
- Specimen drying
- 55 °C for 6 hours in a forced-air oven
- Annealing
- None