PETG-CF
Carbon fibre reinforced filament with a PETG matrix.
- Polymer matrix
- PETG
- Filament diameter
- 1.75 ± 0.03 mm
- Net filament weight
- 1 kg
Price confirmed by quotation
We confirm pricing, supply and sample availability on request.

Application example
Evaluate the jig with the part in place.
A ribbed motor test stand is a sample geometry for reviewing mounting surfaces and access for assembly. Include build orientation, fastening loads and service temperature in your test plan.
- Tensile strength · XY
- 66 ± 2 MPa
- Tensile strength · Z
- 19 ± 1 MPa
- HDT · ISO 75 (1.80 MPa)
- 70.5 °C
Material selection
Compare the technical data.
The supplier reported PETG-CF and PLA-CF results under the same test methods. The specimens were printed at different nozzle and bed temperatures.
| Property and method | PETG-CFAvailable from supplier | PLA-CFAvailable from supplier | PA6-CFIn testing | PPS-CFIn testing |
|---|---|---|---|---|
| Measured properties | ||||
| Tensile strength · XYISO 527 / GB/T 1040 | 66 ± 2 MPa | 50 ± 1 MPa | Data pending | Data pending |
| Tensile strength · ZISO 527 / GB/T 1040 | 19 ± 1 MPa | 17 ± 1 MPa | Data pending | Data pending |
| Flexural modulus · XYISO 178 / GB/T 9341 | 5,825 ± 101 MPa | 6,716 ± 163 MPa | Data pending | Data pending |
| HDTISO 75 · 1.80 MPa | 70.5 °C | 55.3 °C | Data pending | Data pending |
| DensityISO 1183 | 1.265 g/cm³ | 1.289 g/cm³ | Data pending | Data pending |
| Recommended print conditions | ||||
| Nozzle temperature | 230–260 °C | 200–230 °C | Data pending | Data pending |
| Bed temperature | 60–70 °C | 55–65 °C | Data pending | Data pending |
| Drying before printing | 65 °C for 6–12 hours | 55 °C for 6–12 hours | Data pending | Data pending |
HDT measures deflection under the specified load. Validate the part’s service temperature under its intended operating conditions.
Product format
- Filament diameter
- 1.75 ± 0.03 mm
- Net filament weight
- 1 kg
- Packaging
- Vacuum-sealed bag and carton
- Spool material
- Cardboard
- Empty spool weight
- 146 ± 1 g
- Spool dimensions
- Outer Ø 200 mm · inner Ø 88.5 mm · width 65.5 mm
- Carbon fibre content
- 10 %
- Country of origin
- China
Recommended printing settings
- Pre-print drying
- 65 °C for 6–12 hours
- Nozzle temperature
- 230–260 °C
- Bed temperatureTextured PEI plate
- 60–70 °C
- Chamber temperature
- < 50 °C
- Printer type
- Open-frame and enclosed
- Nozzle material
- Hardened steel or tungsten carbide
- Nozzle diameter
- 0.4 / 0.6 / 0.8 mm
- Print speed
- 30–300 mm/s
- Volumetric flow
- 3–32 mm³/s
- Cooling fan speed
- 50–100 %
- Optional annealing
- 65–70 °C for 6–12 hours
Physical and thermal properties
- DensityISO 1183
- 1.265 g/cm³
- Glass transition temperature (Tg)DSC, 10 °C/min
- 77.2 °C
- Vicat softening temperatureISO 306 / GB/T 1633
- 80.7 °C
- Heat deflection temperature (HDT)ISO 75 · 1.80 MPa
- 70.5 °C
- Heat deflection temperature (HDT)ISO 75 · 0.45 MPa
- 71.7 °C
HDT is the deflection temperature measured at the specified test load. Assess suitability under the part’s actual service conditions.
Mechanical properties of printed specimens
- Tensile strength · XYISO 527 / GB/T 1040
- 66 ± 2 MPa
- Tensile strength · ZISO 527 / GB/T 1040
- 19 ± 1 MPa
- Young’s modulus · XYISO 527 / GB/T 1040
- 6,181 ± 122 MPa
- Young’s modulus · ZISO 527 / GB/T 1040
- 1,616 ± 189 MPa
- Elongation at break · XYISO 527 / GB/T 1040
- 2.2 ± 0.2 %
- Elongation at break · ZISO 527 / GB/T 1040
- 2.6 ± 0.3 %
- Flexural strength · XYISO 178 / GB/T 9341
- 96 ± 2 MPa
- Flexural strength · ZISO 178 / GB/T 9341
- 29 ± 1 MPa
- Flexural modulus · XYISO 178 / GB/T 9341
- 5,825 ± 101 MPa
- Flexural modulus · ZISO 178 / GB/T 9341
- 1,354 ± 31 MPa
- Unnotched impact strength · XYISO 179 / GB/T 1043
- 38.3 ± 2.1 kJ/m²
- Notched impact strength · XYISO 179 / GB/T 1043
- 8.2 ± 0.2 kJ/m²
- Impact strength · ZISO 179 / GB/T 1043
- 14.5 ± 1.6 kJ/m²
Reference results from the manufacturer’s data sheet. Values may vary with printer, drying and print settings.
Test specimen preparation
- Printer
- Bambu Lab H2D
- Nozzle temperature
- 255 °C
- Nozzle diameter
- 0.4 mm
- Bed temperature
- 70 °C
- Layer height
- 0.2 mm
- Print speed
- XY 150 mm/s · Z 60 mm/s
- Infill
- 100% · concentric
- Specimen drying
- 55 °C for 6 hours in a forced-air oven
- Annealing
- None